DZˮ¾µ×ÔÕ³ÐÍÒºÌå¹èÏ𽺠MY LSR 3M60
²úÆ·½éÉÜ£º
MY LSR 3M60 A/B ÊÇÒ»ÖÖ¶ÔPC ¾ßÓÐ×ÔÕ³ÌØÐÔµÄÒºÌå¹èÏ𽺣¬Í¬Ê±¾ßÓнϺõÄÀëÄ£ÐÔ¡£
Ö÷ÒªÌØµã:
1.Ë«×é·Ö£¬1:1 »ìºÏ±ÈÀý
2.ÓÅÒìµÄÀëÄ£ÐÔ
3.¶ÔPC¾ßÓÐ׿ԽµÄ×ÔÕ³ÐÔ
4.¿ìËÙÈȹ̻¯
5.ÓÅÒìµÄ»úеÐÔÄÜ
µäÐÍÓ¦Óãº
1.Ó¾¾µÃÜ·â
2.ÊÖ»ú±£»¤¿Ç°ü½º
3.ÖÇÄÜÊÖ±íºó¸ÇÃÜ·âȦ
4.ÊÖ»ú¿¨ÍÐÃÜ·âµÈ
¹Ì»¯
|
ζÈ
|
¹Ì»¯Ê±¼ä£¬1cmºñ¶È
|
|
125¡ãC
|
200 S
|
|
150¡ãC
|
50 S
|
ÖØÒªÊÂÏ
1.MY LSR 3M60 A/B ÊÇʹÓò¬½ð´ß»¯µÄ²úÆ·£¬²¬½ð´ß»¯¼ÁÔÚA ×é·Ö£¬Ê¹ÓÃʱÐèÑϸñ×¢Ò⣬±ÜÃâ´ß»¯¼ÁÖж¾¡£
2.Ö»ÓÐͬÅúºÅµÄA B ×é·Ö²ÅÄÜÒ»Æð»ìºÏʹÓá£
3.Ϊȷ±£ÎïÁϵÄ×î¼ÑÁ÷¶¯ÐԺ;ùÔÈÐÔ£¬ÎïÁÏÔÚ×ªÒÆµ½ÈÝÆ÷ÄÚǰ±ØÐë³ä·Ö½ÁÔÈ¡£
¼¼Êõ²ÎÊý£º
|
ÐÔÄÜ
|
¼ì²â·½·¨
|
ÊýÖµ
|
|
δ¹Ì»¯²úÆ·
|
|
|
|
A ×é·Ö
|
|
|
|
ÑÕÉ«
|
|
͸Ã÷
|
|
ÃÜ¶È 23¡ãC
|
|
1.138 g/cm3
|
|
Õ³¶È 23¡æ£¬10S-1
|
ISO3219
|
300 Pa.s
|
|
B ×é·Ö
|
|
|
|
ÑÕÉ«
|
|
°ë͸Ã÷
|
|
ÃÜ¶È 23¡ãC
|
|
1.138 g/cm3
|
|
Õ³¶È 23¡æ£¬½Á°èºó
|
ISO3219
|
500 Pa.s
|
|
²úÆ·Êý¾Ý£¨A+B »ìºÏ£©
|
|
|
|
»ìºÏ±ÈÀý£¨ÖØÁ¿£©
|
A:B
|
1:1
|
|
Õ³¶È 23¡æ£¬½Á°èºó
|
ISO3219
|
400 Pa.s
|
|
¹Ì»¯Ê±¼ä
|
|
¼û¹Ì»¯Ìõ¼þ
|
|
²úÆ·Êý¾Ý£¨¹Ì»¯ºó£©
|
£¨125¡À2¡ãC£¬Áò»¯200sºó£©
|
|
|
ÑÕÉ«
|
|
͸Ã÷
|
|
ÃÜ¶È 23¡ãC
|
ISO2781
|
1.138 g/cm3
|
|
Ó²¶È
|
DIN 53505
|
60
|
|
ÀÉìÇ¿¶È
|
DIN 53504
|
10MPa
|
|
É쳤ÂÊ
|
DIN 53504
|
450 %
|
|
˺ÁÑÇ¿¶È
|
ASTMD 624B
|
40 KN/m
|
|
PCÄÚ¾ÛÆÆ»µ¡Ý50%
|
/
|
ºÏ¸ñ
|
°ü×°ÐÅÏ¢£º
A ×é·Ö 20 Kg/Ͱ£¬B ×é·Ö 20 Kg/Ͱ¡£
´æ´¢ºÍ±£³ÖÆÚÏÞ£º
µÍÓÚ 23¡æÌõ¼þÏ£¬Î´¿ªÍ°±£´æ 12 ¸öÔ£¬×î¼Ñ½ØÖ¹Ê¹ÓÃÈÕÆÚ±»±ê¼ÇÓÚÿ¸ö²úÆ·Íâ°ü×°µÄ±êÇ©ÉÏ¡£